The butt weld is the most common weld form in steel structures and welded machinery. Load transfer is direct and stress concentration is small, but get one length or one strength grade wrong and the weld may tear from the root. Below we work through a Q345 steel plate butt joint example, then unfold the formulas and parameter tables.
Two Q345 steel plates are butt welded, plate width b = 200mm, plate thickness t = 12mm, carrying an axial tensile force N = 300 kN.
The weld is a grade 3 butt weld (visual inspection only, no NDT), E50 series electrodes, without run-on / run-off plates.
Without run-on / run-off plates, one plate thickness t is deducted at each end of the weld:
For Q345 steel plate, the tensile strength design value of a grade 3 butt weld is f_t^w = 265 MPa (see Table 2).
σ = 142.0 MPa < f_t^w = 265 MPa,the strength is acceptable ✓, with a stress utilisation of about 54%.
| Weld grade | Inspection requirement | Typical application |
|---|---|---|
| Grade 1 weld | Full penetration + 100% non-destructive testing (ultrasonic / radiographic) | Dynamic loads, fatigue-sensitive parts, important locations under direct tension |
| Grade 2 weld | Full penetration + 20% non-destructive testing | Static loads or members under general tension, beam flanges, etc. |
| Grade 3 weld | Visual inspection is sufficient | Members in compression, secondary welds, non-load-bearing connections |
For plate thickness t ≤ 6mm no groove is needed (I-shaped weld, welded from both sides); for t = 6~20mm a V groove is common; for t = 12~40mm use a U groove; for t > 20mm use an X groove (double V). When the thickness difference exceeds the specified limit, the thicker side should be tapered as a transition, with a slope no steeper than 1:2.5.
1. Axial force action (tension / compression):
2. Moment action (butt weld under bending):
3. Shear force action:
4. Combined moment and shear (equivalent stress):
| Symbol | Meaning | Value notes |
|---|---|---|
| l_w | Effective weld length | The actual length with run-on / run-off plates; l − 2t without them |
| t | Effective thickness | The thickness of the thinner of the two butted plates (for unequal thickness, treat it through the groove detail) |
| N | Axial force | Unit N |
| M | Moment | Unit N·mm |
| f_t^w | Tensile strength design value | Look it up by steel grade and weld grade |
| f_v^w | Shear strength design value | Normally taken as the shear design value of the parent metal |
| Steel grade | Weld grade | Tensile f_t^w | Compression f_c^w | Shear f_v^w |
|---|---|---|---|---|
| Q235 | Grade 1, grade 2 | 215 | 215 | 125 (Q235/Q345) 180 (Q390/Q420) |
| Grade 3 | 185 | 215 | ||
| Parent metal | 215 | 215 | ||
| Q345 | Grade 1, grade 2 | 310 | 310 | |
| Grade 3 | 265 | 310 | ||
| Parent metal | 310 | 310 |
| Case | Value of l_w |
|---|---|
| Welded with run-on / run-off plates | The actual weld length l |
| Welded without run-on / run-off plates | l − 2t (deduct t at each end) |
| Slope weld (slope ≤ 1:2) | Calculated along the sloped length; strength verification may be omitted |
| Plate thickness t | Recommended groove | Welding method |
|---|---|---|
| ≤ 6 mm | I shape (no groove) | Welded from both sides |
| 6 ~ 20 mm | V shape (60°) | Single side welding + back gouging |
| 12 ~ 40 mm | U shape / X shape | Welded from both sides |
| > 40 mm | U shape + backing strip | Multi-layer multi-pass welding |
| # | Common error | Consequence | Correct practice |
|---|---|---|---|
| 1 | Taking the full weld length without deducting the defective zones at both ends | The stress is understated and the weld cracks at its ends | Without run-on / run-off plates, l_w = l − 2t |
| 2 | Treating a grade 3 weld as grade 1 and calculating straight from the parent metal strength | The weld fails first, by brittle fracture | The tensile strength design value of a grade 3 weld must be stepped down (Q345: 265 vs 310) |
| 3 | Using the tension formula N/A_w for a weld under bending | The bending normal stress is wrong and the weld tears | For bending use σ = 6M/(t·l_w²); for combined action use the equivalent stress |
| 4 | Butting plates of unequal thickness directly with no taper on the thicker side | Stress concentration and cracking at the weld root | When the thickness difference exceeds the limit, taper the thicker side with a slope ≤1:2.5 |
| 5 | Still using the thin-plate strength value for plate above 16mm | The capacity is overestimated | For grades such as Q345 the strength design value must be reduced with thickness when t>16mm |