Chemical composition per GB/T 3077 standard range (reliability: high); mechanical properties are typical values / ranges (reliability: medium) — acceptance is governed by the purchase standard and the mill test certificate.
| C | 0.17~0.24 |
| Cr | 0.70~1.00 |
| Mo | 0.20~0.30 |
| Condition | Tensile MPa | Yield MPa | Elong. % | Hardness |
|---|---|---|---|---|
| Quenched + tempered | ≥885 | ≥685 | ≥12 | ≤180HB (before carburizing) |
Carburizing: 920–940°C, quench + temper at 180–200°C. Case depth 0.6–1.2 mm.
Medium-load carburized gears, piston pins, cams. The Mo-series substitute for 20CrMnTi.
20CrMnTi carburizing gear steel (GB) 20Cr (AISI 5120) alloy steel