Chemical composition per GB/T 1222 standard range (reliability: high); mechanical properties are typical values / ranges (reliability: medium) — acceptance is governed by the purchase standard and the mill test certificate.
| C | 0.62~0.70 |
| Si | 0.17~0.37 |
| Mn | 0.90~1.20 |
| Condition | Tensile MPa | Yield MPa | Elong. % | Hardness |
|---|---|---|---|---|
| Quenched + medium-temp tempered | ≥1000 | ≥800 | — | approx. 42~48HRC |
Oil quench at 830°C, medium-temperature temper around 480°C (to obtain the highest elastic limit). Annealed state ≤285 HB for easy stamping forming.
Spring washers, circlips, spring wire, agricultural blades, and massage-chair springs. A cheap, readily available spring steel.