Chemical composition per GB/T 3077 standard range (reliability: high); mechanical properties are typical values / ranges (reliability: medium) — acceptance is governed by the purchase standard and the mill test certificate.
| C | 0.37~0.44 |
| Si | 0.17~0.37 |
| Mn | 0.50~0.80 |
| Cr | 0.80~1.10 |
| Condition | Tensile MPa | Yield MPa | Elong. % | Hardness |
|---|---|---|---|---|
| Q&T (test bar 25mm) | ≥980 | ≥785 | ≥9 | 217~286HB |
| Q&T + surface hardening | — | — | — | surface 48~55HRC |
Q&T: oil quench at 850°C, temper at 520~580°C. Surface induction hardening plus low-temperature tempering for journals/gear faces.
Medium-load shafts, gears, worms, connecting rods, and important bolts. The first upgrade when 45 steel is "not hard/tough enough or not deep enough."
42CrMo4 (AISI 4140) alloy steel C45 (AISI 1045) carbon steel 34CrMo4 (AISI 4135) alloy steel