Electrode grades (GB trade names) for common base metals; for welding procedure cards and site issuance.
| Base metal | Electrode grade | Trade no. | Note |
|---|---|---|---|
| Q235 mild steel | E4303 | J422 | Most common acidic electrode |
| Q235 (critical structure) | E4315/E4316 | J427/J426 | Basic; better toughness |
| Q345/16Mn | E5015/E5016 | J507/J506 | Basic low-hydrogen |
| 45 medium-carbon steel | E5015 | J507 | Preheat 250-300 C, slow cool after weld |
| 304 stainless steel | E308-16 | A102 | — |
| 316 stainless steel | E316-16 | A202 | — |
| Grey cast iron repair | EZNi/EZC | Z308/Z208 | Ni-base, machinable; low current, skip welding |
45 steel welds poorly (high carbon equivalent): must preheat + post-weld temper; bolt instead of weld if possible. Stainless electrodes match the base – 'equal or higher, never lower' (don't use 308 on 316 base metal).
See all quick calculators on the knowledge base home page.
Data compiled from publicly available GB/T standard tables for design reference only. For final design and acceptance, always consult the original standard and the latest supplier catalog.