Chemical composition per GB/T 699 standard range (reliability: high); mechanical properties are typical values / ranges (reliability: medium) — acceptance is governed by the purchase standard and the mill test certificate.
| C | 0.42~0.50 |
| Si | 0.17~0.37 |
| Mn | 0.50~0.80 |
| Condition | Tensile MPa | Yield MPa | Elong. % | Hardness |
|---|---|---|---|---|
| Normalized | ≥600 | ≥355 | ≥16 | ≤229HB |
| Q&T | approx. 650~800 | approx. 380~550 | ≥17 | 217~255HB |
| Quenched + low-temp tempered | — | — | — | surface approx. 45~52HRC |
Normalizing: 830~860°C air cooling. Q&T: water quench around 840°C (oil quench for small parts), temper at 560~600°C. Induction hardening can reach 52~58 HRC on the surface.
The "all-round" steel for custom design: shafts, gears, lead screws, keys, worms, jig bodies, and templates. The default choice when no special requirements exist.
41Cr4 (AISI 5140) alloy steel 42CrMo4 (AISI 4140) alloy steel AISI 1035 carbon steel (GB 35)