Chemical composition per GB/T 699 standard range (reliability: high); mechanical properties are typical values / ranges (reliability: medium) — acceptance is governed by the purchase standard and the mill test certificate.
| C | 0.57~0.65 |
| Si | 0.17~0.37 |
| Mn | 0.50~0.80 |
| Condition | Tensile MPa | Yield MPa | Elong. % | Hardness |
|---|---|---|---|---|
| Normalized | ≥675 | ≥400 | ≥12 | ≤255HB |
| Quenched + tempered (medium) | — | — | — | ≈40~50HRC |
Oil quench around 810°C (water quench cracks easily), temper at 450–500°C.
Flat springs, washers, circlips, wear parts. A high-carbon steel harder and with higher elastic limit than 55 steel.
65Mn spring steel (GB) GB 55 carbon steel (AISI 1055)