MOULDLKnowledge Base3D Model DownloadsMembership
中文版Model Store »
Knowledge Base › General Engineering & Case Studies › Why Hardness Conversions Never
HomeModels
Table of contents

General Engineering & Case Studies (60 articles)

Knowledge Base Home

📐 Standard Data

🧮 Calculators

📖 Selection Guides

🏭 Material Grades

❓ Engineer FAQ

🗂 Quick-Reference Categories

❌ Error Case Studies

📚 Technical Articles

Why Hardness Conversions Never Line Up: Brinell, Rockwell and Vickers Tables with a Complete Example

🛠️ Baisi Technical Handbook · Intelligent selection and calculation for 500+ standard parts
Covers the full range of pneumatic / motor / power transmission / reducer / coupling / bearing / hydraulic / pneumatic / thread / worm / spring parts
Avoid 95% of design errors, improve design efficiency by 80%
Master 10 years of senior engineer experience in 3 months
Download: https://pan.baidu.com/s/1bquayZpfas6oYBbG0gp3Gw?pwd=2giv

📖 Next issue: The Digital Knowledge Base of Mechanical Engineering

The step where incoming inspection most often gets stuck is not that the value cannot be measured, but that the measured value cannot be compared directly. The drawing says HRC and the shop only has a Brinell tester; the Vickers gradient comes out but the acceptance criterion is in Rockwell. The indenter shape, the test force and the indentation depth of the three scales are all different, and comparing the numbers side by side is like measuring the same shaft in meters and in feet.

Below we work through a complete inspection case of a carburised and hardened gear, then expand into the formulas and the conversion tables.

I. Complete Worked Example: Three Judgements of a 20CrMnTi Carburised Gear

Known conditions

ItemDrawing requirementMeasured data
Tooth flank hardness58 ~ 62 HRC60.5 HRC (Rockwell C scale)
Core hardness30 ~ 42 HRC302 HB (Brinell 3000 kgf)
Effective case depth0.8 ~ 1.2 mm (referenced to 550 HV1)0.2mm:720 HV1|0.6mm:610 HV1|1.0mm:560 HV1|1.4mm:480 HV1
Core tensile strength≥ 980 MPaBack-calculated from hardness
Step 1 — Unify the reference scale: Rockwell converted to Vickers

Vickers hardness has a small indentation, is sensitive to thin layers and gradients, and is the general reference for carburised parts. Look up the ASTM E140 conversion table: HRC 60 = HV 697, HRC 61 = HV 720.

Linear interpolation: 697 + (720 − 697) × (60.5 − 60) / (61 − 60) = 697 + 23 × 0.5 = 708.5

Tooth flank = HV 708

Step 2 — Core Brinell converted to Rockwell

Look up the table: HB 301 = HRC 32, HB 311 = HRC 33; between these two points every 10 HB corresponds to 1 HRC.

32 + (302 − 301) / (311 − 301) × (33 − 32) = 32.1

Core = HRC 32.1, the drawing requires 30 ~ 42 HRC, so it falls in the middle of the range.

Step 3 — Effective case depth (550 HV1 reference point)

In the gradient data the value at 1.0 mm is 560 HV1 and at 1.4 mm it is 480 HV1, so the 550 HV1 reference point lies between these two points.

CHD = 1.0 + (560 − 550) / (560 − 480) × (1.4 − 1.0) = 1.0 + 0.125 × 0.4 = 1.05

Effective case depth = 1.05 mm, against a requirement of 0.8 ~ 1.2 mm.

Step 4 — The three-item pass judgement
ItemMeasured (after unification)Required rangeConclusion
Tooth flank hardness60.5 HRC = 708 HV58 ~ 62 HRCPass ✓
Core hardnessHB 302 = 32.1 HRC30 ~ 42 HRCPass ✓
Effective case depth1.05 mm0.8 ~ 1.2 mmPass ✓

All three pass, so this batch can be released.

Step 5 — Back-calculating the tensile strength from the hardness

Carbon steel and low-alloy steel have a well-established empirical relation: σb ≈ 3.3 × HB (MPa).

σb = 3.3 × 302 = 996.6 ≈ 997 MPa

The core strength requirement is ≥ 980 MPa, so the margin is only 1.7%. As soon as the material batch or the tempering temperature drifts, the core can drop below the required line — which is why hardness must not be checked only against the "pass" lower limit; the margin matters too.

Step 6 — Rockwell indentation depth and minimum test piece thickness

Each division of the Rockwell C scale corresponds to an indentation depth of 0.002 mm:

h = (100 − HRC) × 0.002 = (100 − 60.5) × 0.002 = 0.079 mm

By the ten-times rule, the test piece thickness must be at least 10 h = 0.79 mm. The effective section of the gear is far greater than this, so the indentation will not be affected by the base support effect.

Thin-walled sleeves, gaskets and tool coatings are often where this step bites: if the test piece is too thin, the measured hardness reads 2 ~ 5 units low and the part is wrongly judged non-conforming.
Step 7 — Scale and equipment selection
Inspection objectRecommended scaleExplanation
Hardened parts HRC ≥ 20Rockwell C (HRC)150 kgf diamond cone
Soft steel HRC < 20Rockwell B (HRB)100 kgf steel ball; the C scale no longer applies
Thin parts / shallow caseSurface Rockwell HR15N / HR30N15 / 30 kgf, shallower indentation
Case gradientVickers HV1 / HV0.51 / 0.5 kgf, small indentation
Annealed, normalised, quenched and tempered partsBrinell HBWLarge indentation, highly representative
Large parts on siteLeeb HLMust be calibrated on standard test blocks; the error can reach ±2 HRC
📘 Baisi Technical Handbook
The Baisi Technical Handbook has integrated this calculation module into the Group 0 Basic Tools calculation module. Enter the duty parameters and it automatically outputs the selection result. Say goodbye to paging through handbooks, to hand calculations and to rule-of-thumb estimates.
—— Baisi Technical Handbook download https://pan.baidu.com/s/1bquayZpfas6oYBbG0gp3Gw?pwd=2giv

II. Classification and Applicability Boundaries of the Hardness Scales

1. Classified by indenter and test force

ScaleIndenterTest forceApplicable hardness rangeTypical use
Rockwell C (HRC)120° diamond cone150 kgf20 ~ 67 HRCHardened steel, carburised parts
Rockwell B (HRB)φ1.588 mm steel ball100 kgf20 ~ 100 HRBSoft steel, copper alloys, annealed parts
Rockwell A (HRA)Diamond cone60 kgf60 ~ 88 HRAHard alloys, thin carburised layers
Surface Rockwell (HR15N)Diamond cone15 kgf—Thin parts, platings, nitrided layers
Brinell (HBW)Carbide ball3000 / 750 / 187.5 kgf< 650 HBWAnnealed, normalised, quenched and tempered, castings
Vickers (HV)Diamond square pyramid1 ~ 100 kgfFull rangeCase gradients, thin parts, arbitration
Leeb (HL)Carbide ball impactorImpact rebound—Large parts on site, immovable parts

2. Why the different scales cannot be compared directly

Rockwell uses the difference in indentation depth, Brinell and Vickers use the indentation area, and Leeb uses the ratio of rebound velocities. The physical quantities and dimensions differ, and forcing the numbers side by side yields nothing but an illusion.

The three can only be related empirically through standard conversion tables, and this relation holds only for steel. Cast iron, aluminium alloys, copper alloys and hard alloys each have their own dedicated tables, and mixing them gives errors of 5 ~ 10 units.

III. Core Calculation Formulas

1. Two-point linear interpolation conversion

X = X₁ + (Y − Y₁) / (Y₂ − Y₁) × (X₂ − X₁)

X is the value to be found in the target scale, Y is the known value, and subscripts 1 and 2 denote the two points in the conversion table immediately adjacent to the known value. Both the HRC→HV and the HB→HRC conversions in this example use this expression.

2. Rockwell indentation depth and minimum test piece thickness

h = (100 − HRC) × 0.002 mm  tmin ≥ 10 h

The dividing principle of the Rockwell C scale is the indentation depth: each 0.002 mm of depth difference corresponds to one Rockwell unit. The higher the HRC, the shallower the indentation. When the test piece is thinner than ten times the indentation depth, the base support effect distorts the reading.

3. Back-calculating tensile strength from hardness (steel)

σb ≈ 3.3 × HB (MPa, carbon steel and low-alloy steel)

This relation applies to quenched and tempered or normalised steel with HB between 150 and 450. It does not hold for hardened martensite, austenitic stainless steel or cast iron; use the corresponding empirical coefficients or carry out a tensile test directly.

4. Effective case depth (CHD)

CHD = d₁ + (HV₁ − HVlim) / (HV₁ − HV₂) × (d₂ − d₁)

d₁ and d₂ are the depths of two adjacent measurement points that straddle the reference hardness HVlim, and HV₁ and HV₂ are the corresponding hardness values. For carburised parts the reference hardness is usually 550 HV1, and for nitrided parts 400 HV0.3 (depending on the standard).

IV. Common Conversion Tables and Parameter Selection Guide

1. Rockwell / Vickers / Brinell comparison (steel, excerpt of ASTM E140)

HRCHVHBW (3000 kgf)Typical corresponding condition
20238226Quenched and tempered
25266253Quenched and tempered
30302286Quenched and tempered / core
35345327Quenched and tempered / core
40392371Induction hardened
45446421Induction hardened
50513481Hardened + low-temperature tempered
55595560Hardened + low-temperature tempered
60697654Carburised and hardened / bearing steel
62746706Carburised and hardened / bearing steel

2. Hardness versus tensile strength (σb ≈ 3.3 HB)

HBWEstimated σb (MPa)Approximately corresponds to HRC
150495—
200660≈ 10
250825≈ 22
300990≈ 32
3501155≈ 38
4001320≈ 43

3. Common hardness and case depth parameters for carburised and nitrided parts

ProcessSurface hardnessCore hardnessEffective case depthReference hardness
Carburising and hardening (gears)58 ~ 62 HRC30 ~ 42 HRC0.8 ~ 1.2 mm550 HV1
Carburising and hardening (heavy duty)58 ~ 63 HRC30 ~ 45 HRC1.2 ~ 2.0 mm550 HV1
Gas nitriding≥ 650 HVQuenched and tempered state0.3 ~ 0.5 mm400 HV0.3
Plasma nitriding≥ 700 HVQuenched and tempered state0.2 ~ 0.4 mm400 HV0.3
Induction hardening55 ~ 62 HRCQuenched and tempered state1.0 ~ 4.0 mm0.8 × surface hardness

4. Key points on parameter selection

Selection itemRecommended practiceReason
Vickers test forceFor a case ≤ 0.5 mm use HV0.3 ~ HV1A large test force gives a deep indentation that penetrates the case
Number of pointsAt least 3 points on the same part, take the averageMicrostructure is non-uniform and a single point can scatter by ±2 HRC
Inspection locationMeasure the tooth tip, the tooth root and the core separatelyThe tooth tip and the tooth root can differ by 3 HRC
Surface preparationRemove the oxide scale, Ra ≤ 1.6 μmA rough surface reads low
Arbitration standardState ASTM E140 / ISO 18265 / GB/T 1172 on the drawingDifferent conversion tables differ by 1 ~ 2 HRC

V. Common Errors and How to Avoid Them

Common errorConsequenceCorrect practice
Comparing Rockwell and Brinell values directlyTreating 302 HB as 302 HRC, and the judgement goes completely off trackUnify to the same scale before comparing
Using a conversion table without regard to the materialErrors of 5 ~ 10 units for cast iron and aluminium alloysUse the dedicated table for the corresponding material
Choosing too large a Vickers test forceThe indentation penetrates the case and the core is measured insteadUse HV0.3 ~ HV1 for the case
Looking at a single point and not at the locationSoft spots are missed and early pitting failure occursMeasure 3 points each on the tooth tip, the tooth root and the core
Using Rockwell C directly on thin partsBase support effect makes the reading 2 ~ 5 units lowWhen the thickness is < 10h use surface Rockwell or Vickers
Not specifying the standard for arbitrationThe supplier's and the customer's data do not agree and the argument drags onState the conversion standard and its version on the drawing
Remember it in one sentence: unify the scale first, compare the numbers second, and check the standard and the inspection location last. A hardness conversion table is an empirical correspondence, not a physical identity — it helps you to judge, but it cannot decide for you whether the part is acceptable.

Summary

Hardness conversion looks like nothing more than looking up a table, but the real hurdle is knowing which table can be used and which cannot. Steel has its table, cast iron has its own; a case needs a small test force and a thin part needs surface Rockwell; and a judgement must look at the tooth flank, the core and the case depth together — no single one of them passing means the part is acceptable.

Make these three steps part of the routine and at least half of the disputes in incoming inspection disappear.

Related 3D models: Ready to build it? Download free 3D models & CAD drawings at MOULDL »