Chemical composition per GB/T 3077 standard range (reliability: high); mechanical properties are typical values / ranges (reliability: medium) — acceptance is governed by the purchase standard and the mill test certificate.
| C | 0.26~0.34 |
| Si | 0.17~0.37 |
| Mn | 0.40~0.70 |
| Cr | 0.80~1.10 |
| Mo | 0.15~0.25 |
| Condition | Tensile MPa | Yield MPa | Elong. % | Hardness |
|---|---|---|---|---|
| Q&T (specimen 25 mm) | ≥930 | ≥785 | ≥12 | ≈207~241HB |
Q&T: oil quench around 860°C, temper at 540–580°C.
Medium-strength shafts, boiler / high-temperature fasteners (≤450°C), pipe fittings. The lower-spec sibling of 35CrMo.
34CrMo4 (AISI 4135) alloy steel 41Cr4 (AISI 5140) alloy steel