Yield/tensile strength and hardness of structural steels, cast iron and stainless steel for material selection and static strength check.
| Grade | Condition | Yield σs (MPa) ≥ | Tensile σb (MPa) ≥ | Hardness (HB) ref. |
|---|---|---|---|---|
| Q235A | Hot rolled | 235 | 370~500 | — |
| 35 | Normalized | 315 | 530 | ≤187 |
| 45 | Normalized | 355 | 600 | ≤217 |
| 45 | Quenched and tempered | — | ≥600 | 217~255 |
| 40Cr | Quenched and tempered | 785 | 980 | 207~255 |
| 42CrMo | Quenched and tempered | 930 | 1080 | 217~269 |
| 20Cr | Carburized and quenched | 540 | 835 | Tooth surface 56~62HRC |
| 65Mn | Quenched + medium-temperature tempered | 430 | 735 | — |
| 60Si2Mn | Quenched + medium-temperature tempered | 1176 | 1275 | — |
| ZG270-500 | Normalized | 270 | 500 | — |
| HT200 | — | — | 200 (tensile) | — |
| QT450-10 | — | 310 | 450 | 160~210 |
| 304 | Solution treated | 205 | 520 | ≤187 |
| 316 | Solution treated | 170 | 480 | ≤187 |
These are reference values for normal loading; in practice, verify against the material mill certificate and batch re-inspection; the tensile strength concept σs does not apply to cast iron.
See all quick calculators on the knowledge base home page.
Data compiled from publicly available GB/T standard tables for design reference only. For final design and acceptance, always consult the original standard and the latest supplier catalog.