Chemical composition per GB/T 3077 standard range (reliability: high); mechanical properties are typical values / ranges (reliability: medium) — acceptance is governed by the purchase standard and the mill test certificate.
| C | 0.35~0.42 |
| Si | 0.20~0.45 |
| Mn | 0.30~0.60 |
| Cr | 1.35~1.65 |
| Mo | 0.15~0.25 |
| Al | 0.70~1.10 |
| Condition | Tensile MPa | Yield MPa | Elong. % | Hardness |
|---|---|---|---|---|
| Q&T + nitriding | — | ≥835 (core) | — | surface ≥950HV (approx. 68HRC) |
Q&T (oil quench at 930°C + temper at 620°C) → finish machining → nitride at 510~540°C for 30~60 h.
Main shafts, lead screws, precision gears, and other parts requiring extremely hard surfaces with minimal distortion. Nitriding temperature is low (<540°C), so distortion is negligible.
42CrMo4 (AISI 4140) alloy steel 20CrMnTi carburizing gear steel (GB)