Chemical composition per GB/T 1299 standard range (reliability: high); mechanical properties are typical values / ranges (reliability: medium) — acceptance is governed by the purchase standard and the mill test certificate.
| C | 0.32~0.45 |
| Cr | 4.75~5.50 |
| Mo | 1.10~1.75 |
| V | 0.80~1.20 |
| Si | 0.80~1.20 |
| Condition | Tensile MPa | Yield MPa | Elong. % | Hardness |
|---|---|---|---|---|
| Quenched + double tempered | — | — | — | working hardness 44~52HRC |
Oil quench / gas quench at 1020~1050°C, two tempers at 600°C + 580°C (2 h each). Delivered isothermally spheroidizing-annealed.
Die-casting dies, hot-forging dies, hot-extrusion dies, and injection-mold cores. A globally common hot-work die steel (US grade H13).
Cr12MoV cold-work die steel (GB)