Chemical composition per GB/T 699 standard range (reliability: high); mechanical properties are typical values / ranges (reliability: medium) — acceptance is governed by the purchase standard and the mill test certificate.
| C | 0.17~0.24 |
| Si | 0.17~0.37 |
| Mn | 0.35~0.65 |
| Condition | Tensile MPa | Yield MPa | Elong. % | Hardness |
|---|---|---|---|---|
| Normalized | ≥410 | ≥245 | ≥25 | ≤156HB |
| Carburized + quenched | surface 56~62HRC | — | — | core approx. 180~250HB |
Normalizing: 910°C air cooling. Carburizing: carburize at 920~940°C followed by direct quenching and low-temperature tempering at 180~200°C.
Carburized gears, piston pins, bushings, and low-pressure piping. A classic low-carbon steel for "hard surface, tough core" parts.
20CrMnTi carburizing gear steel (GB) C45 (AISI 1045) carbon steel 08F rimmed carbon steel (GB)