Chemical composition per GB/T 1299 standard range (reliability: high); mechanical properties are typical values / ranges (reliability: medium) — acceptance is governed by the purchase standard and the mill test certificate.
| C | 1.45~1.70 |
| Cr | 11.0~12.5 |
| Mo | 0.40~0.60 |
| V | 0.15~0.30 |
| Condition | Tensile MPa | Yield MPa | Elong. % | Hardness |
|---|---|---|---|---|
| Quenched + low-temp tempered | — | — | — | 58~62HRC |
| Quenched + high-temp tempered (secondary hardening) | — | — | — | approx. 58~60HRC |
Oil quench / stage quench at 1000~1040°C, low-temperature temper at 200°C (conventional) or three high-temperature tempers at 500°C (when hot hardness is required).
Stamping dies, blanking dies, cold-heading dies, drawing dies, and thread-rolling rings. The default domestic choice for cold-work dies.
AISI H13 hot-work die steel (GB 4Cr5MoSiV1) AISI W1-1.0C (GB T10) tool steel