Chemical composition per GB/T 1299 standard range (reliability: high); mechanical properties are typical values / ranges (reliability: medium) — acceptance is governed by the purchase standard and the mill test certificate.
| C | 0.50~0.60 |
| Cr | 0.50~0.80 |
| Ni | 1.40~1.80 |
| Mo | 0.15~0.30 |
| Condition | Tensile MPa | Yield MPa | Elong. % | Hardness |
|---|---|---|---|---|
| Quenched + tempered | — | — | — | Die face 38~46HRC (approx., tough core) |
Oil quench at 840~860°C, temper around 500°C. Large forging dies must be heated slowly to avoid cracking.
Large hot-forging dies, hot trimming dies. Ni provides core toughness to withstand repeated impact.
AISI H13 hot-work die steel (GB 4Cr5MoSiV1) Cr12MoV cold-work die steel (GB)