Recommended ranges of turning/milling cutting speed vc and feed f for common engineering materials under different carbide grades, for setting cutting parameters.
| Work material | Tool grade | Turning vc (m/min) approx | Milling vc (m/min) approx | Feed f (mm/r) approx | Remarks |
|---|---|---|---|---|---|
| C45 steel (normalized) | YT15 | 120~180 | 60~100 | 0.2~0.4 | Rough turning |
| C45 steel (quenched and tempered) | YT15 | 80~120 | 40~70 | 0.15~0.3 | |
| C45 steel | YW1 | 100~150 | 50~90 | 0.2~0.4 | General |
| 40Cr (quenched and tempered) | YT15 | 70~110 | 40~70 | 0.15~0.3 | |
| 40Cr | YW2 | 80~120 | 45~80 | 0.15~0.3 | |
| Cast iron HT250 | YG8 | 60~100 | 40~70 | 0.2~0.5 | |
| Cast iron HT250 | YG3X | 80~130 | 50~90 | 0.15~0.4 | Finish machining |
| Stainless steel 304 | YW1 | 50~90 | 30~60 | 0.1~0.25 | Prone to built-up edge |
| Stainless steel 304 | YG8 | 40~80 | 25~50 | 0.1~0.2 | |
| Aluminium alloy 6061 | YG3X | 300~600 | 200~400 | 0.1~0.4 | |
| Aluminium alloy 6061 | PCD | 800~1500 | 500~1000 | 0.05~0.3 | Diamond |
| Brass H62 | YG8 | 150~300 | 100~200 | 0.15~0.4 | |
| Titanium alloy TC4 | YW1 | 30~60 | 20~40 | 0.05~0.15 | Difficult to machine |
| Titanium alloy TC4 | K10 | 40~70 | 25~50 | 0.05~0.15 | |
| Hardened steel HRC50 | CBN | 60~120 | 40~80 | 0.1~0.2 | Cubic boron nitride (CBN) |
| Hardened steel HRC55 | CBN | 50~100 | 30~60 | 0.08~0.15 | |
| Cast steel ZG | YG8 | 50~90 | 35~60 | 0.2~0.4 | |
| Superalloy GH | K20 | 15~35 | 10~25 | 0.05~0.1 | Nickel-based |
| Chilled cast iron | CBN | 40~80 | 30~60 | 0.1~0.2 | |
| Ductile iron QT | YG8 | 70~120 | 50~90 | 0.2~0.4 | |
| C45 steel (normalized) | YT5 | 80~140 | 50~90 | 0.3~0.5 | Heavy depth of cut |
| 40Cr (quenched and tempered) | YT14 | 70~110 | 40~70 | 0.15~0.3 | |
| Stainless steel 304 | YS8 | 40~80 | 25~50 | 0.1~0.2 | |
| Aluminium alloy 7075 | YG3X | 300~550 | 200~380 | 0.1~0.4 | |
| Superalloy GH | YS2 | 12~30 | 8~20 | 0.04~0.08 | |
| Hardened steel HRC45 | CBN | 70~130 | 50~90 | 0.1~0.2 | |
| Grey cast iron HT200 | YG8 | 70~110 | 50~90 | 0.2~0.5 | |
| Copper T2 | YG6 | 150~250 | 100~180 | 0.15~0.4 | |
| Magnesium alloy AZ91 | YG3X | 300~600 | 200~400 | 0.1~0.3 | |
| Bearing steel GCr15 | CBN | 60~120 | 40~80 | 0.1~0.2 | Use YT in annealed state |
| 20 steel (carburized) | YT15 | 120~180 | 60~100 | 0.2~0.4 | |
| Q235 | YT15 | 120~200 | 70~110 | 0.2~0.5 | |
| Mold steel P20 | YW2 | 60~100 | 40~70 | 0.15~0.3 | |
| Nylon / plastic | YG8 | 200~500 | 150~350 | 0.1~0.4 | |
| Graphite | K10 | 60~120 | 50~100 | 0.1~0.3 | |
| High-manganese steel ZGMn13 | YW1 | 20~40 | 15~30 | 0.1~0.2 | Work hardening |
| Martensitic stainless steel 420 | YW2 | 50~90 | 30~60 | 0.1~0.2 | |
| Tin bronze | YG8 | 80~150 | 60~120 | 0.15~0.4 | |
| Titanium alloy TA2 | K10 | 40~70 | 25~50 | 0.05~0.15 | |
| 35CrMo (quenched and tempered) | YT14 | 70~110 | 40~70 | 0.15~0.3 |
vc is a recommended range, actually limited by machine rigidity, cooling and tool wear; for hard/difficult materials take the lower limit, combined with calc-21 for quick calculation. Soft materials such as aluminium/copper may use high speed but watch built-up edge.
See all quick calculators on the knowledge base home page.
Data compiled from publicly available GB/T standard tables for design reference only. For final design and acceptance, always consult the original standard and the latest supplier catalog.