MOULDLKnowledge Base3D Model DownloadsMembership
中文版Model Store »
Knowledge Base › General Engineering & Case Studies › How to Look Up Material Mechan
HomeModels
Table of contents

General Engineering & Case Studies (60 articles)

Knowledge Base Home

📐 Standard Data

🧮 Calculators

📖 Selection Guides

🏭 Material Grades

❓ Engineer FAQ

🗂 Quick-Reference Categories

❌ Error Case Studies

📚 Technical Articles

How to Look Up Material Mechanical Properties: Strength of 45 Steel, Q235 and 40Cr Explained in One Go

🛠️ Baisi Technical Handbook · Intelligent selection and calculation for 500+ standard parts
Covers the full range of pneumatic / motor / power transmission / reducer / coupling / bearing / hydraulic / pneumatic / thread / worm / spring parts
Avoid 95% of design errors, improve design efficiency by 80%
Master 10 years of senior engineer experience in 3 months
Download: https://pan.baidu.com/s/1bquayZpfas6oYBbG0gp3Gw?pwd=2giv

📖 Next issue: Geometric Tolerances — How to Mark and Select Them

The drawing says one line, "material 45 steel", but to run a verification you need tensile strength, yield strength, fatigue limit, elastic modulus and hardness — and these data are scattered over dozens of tables in the handbook. Get one number wrong and the whole calculation is wasted. Below we run the whole chain, "look up the database → calculate the allowable stress → verify → select the material", for a lifting tie rod.

I. Complete Worked Example: Material Selection and Strength Verification of a Lifting Tie Rod

Duty condition: the tie rod of a lifting device works with a fluctuating tensile load of 50~250 kN, 8 hours a day, with a required life of no less than 1 million cycles; the rod body is initially φ40, with threaded connections at both ends. Determine the material grade and the heat treatment condition.

Step 1: Determine the failure mode first, then decide which figures to look up

Fluctuating tension-compression → there are two failure modes: yield on first overload (occurring at the first load application) and fatigue fracture (occurring after a million cycles). So four figures are needed: tensile strength σb, yield strength σs, fully reversed fatigue limit σ-1 and elastic modulus E.

Verification targets: static strength safety factor n_s ≥ 1.5; fatigue safety factor n_f ≥ 1.5.

Step 2: Consult the material database and take three candidate grades
Grade / conditionσb (MPa)σs (MPa)σ-1 tension-compression (MPa)E (MPa)HB
Q235B normalised4002351192.06×10⁵≤156
45 steel quenched and tempered6503601902.06×10⁵217~255
40Cr quenched and tempered9807852802.06×10⁵241~286

Three points to note: ① for the same grade with different heat treatment, σs can differ by a factor of 2~3, so the condition must be looked up together with the grade; ② the table gives the tension-compression fatigue limit — the bending fatigue limit is about 1.4 times higher; ③ the E of all three steels is identical, so changing the grade cannot change the stiffness.

Step 3: Choose the safety factor and calculate the allowable stress

[σ] = σs / n_s = 360 / 1.5 = 240 MPa (45 steel, quenched and tempered)

Static loading, accurately calculated load, mature experience → take n_s = 1.5; this lifting device is an important application, so 1.5 is already on the strict side and is not reduced further.

Step 4: First trial-calculate with the cheapest material, Q235B, φ40

A = π×40²/4 = 1257 mm²
σmax = 250000 / 1257 = 198.9 MPa
n_s = 235 / 198.9 = 1.18 < 1.5 ✗

It does not even pass the static strength check, so Q235B is eliminated outright. This step is crucial — trialling with the cheap material first and only upgrading when it fails saves far more than starting with an expensive grade.

Step 5: Switch to 45 steel quenched and tempered, keeping the section at φ40

n_s = 360 / 198.9 = 1.81 ≥ 1.5 ✓
σmin = 50000 / 1257 = 39.8 MPa
σm = (198.9 + 39.8)/2 = 119.4 MPa
σa = (198.9 − 39.8)/2 = 79.6 MPa

Static strength passes, but fatigue has not yet been checked. Substituting into the Soderberg equation:

σa/σ-1 + σm/σs = 79.6/190 + 119.4/360
= 0.419 + 0.332 = 0.751
n_f = 1 / 0.751 = 1.33 < 1.5 ✗

Static strength passes, fatigue fails — this is the most common failure point for parts under alternating load. Although the stress amplitude σa of the fluctuating cycle is only 79.6 MPa, the fatigue limit σ-1 is only 190 MPa, so the margin is not generous.

Step 6: Increase the rod body to φ45 and re-verify

A = π×45²/4 = 1590 mm²
σmax = 157.2 MPa, σmin = 31.4 MPa
σm = 94.3 MPa, σa = 62.9 MPa
n_s = 360 / 157.2 = 2.29 ✓
n_f = 1/(62.9/190 + 94.3/360) = 1/0.593 = 1.69 ✓

Increasing the section from φ40 to φ45 (area +26%) reduces the stress amplitude by 21% and raises the fatigue safety factor from 1.33 to 1.69, so both checks now pass.

Step 7: Compare the 40Cr weight-saving option and confirm the final material

If 40Cr quenched and tempered is used instead, keeping φ40:

n_s = 785 / 198.9 = 3.95 ✓
n_f = 1/(79.6/280 + 119.4/785)
= 1/0.436 = 2.29 ✓

The strength margin is ample and it is about 21% lighter than the φ45 option, but the material plus quenching and tempering costs about 1.9 times that of 45 steel. The trade-off rule: large batches and weight-sensitive applications (long strokes, frequent reciprocation, moving parts) → choose 40Cr φ40; cost-driven, small batches and single pieces → choose 45 steel quenched and tempered at φ45.

Final selection: 45 steel quenched and tempered (HB 217~255), rod body φ45, threaded section M42×3, transition fillet above R5 with roll strengthening.

🛠️ Stop paging through the material handbook page by page

The Baisi Technical Handbook has integrated this calculation module into the Group 0 Basic Tools calculation module. Enter the grade and the heat treatment condition, and it automatically outputs σb, σs, σ-1, E, HB and the allowable stress. Say goodbye to paging through handbooks, to hand calculations and to rule-of-thumb estimates. —— Baisi Technical Handbook download https://pan.baidu.com/s/1bquayZpfas6oYBbG0gp3Gw?pwd=2giv

II. What Data the Material Property Database Actually Contains

PropertySymbol / unitMain useTypical pattern of values
Tensile strengthσb / MPaJudging brittle fracture, estimating the fatigue limitCarbon steel 400~1000, alloy steel up to 1200+
Yield strengthσs / MPaThe core of static strength verification for ductile materialsAbout 0.5~0.7 of σb
Fatigue limitσ-1 / MPaStrength verification under alternating loadBending about 0.4~0.5σb; for tension-compression multiply by 0.7
Elastic modulusE / MPaStiffness, deformation and buckling calculationsSteel 2.06×10⁵, cast iron 1.2×10⁵, aluminium 0.7×10⁵
HardnessHB / HRCWear resistance, machinability, heat treatment criteria45 steel quenched and tempered 217~255HB; hardened 45~55HRC
Elongation / impact energyδ / %, Akv / JDuctility, toughness, assessment of low-temperature brittle fractureStructural parts δ≥5%, at −20℃ Akv≥27J
Densityρ / kg·m⁻³Weight, moment of inertia, centrifugal forceSteel 7850, cast iron 7200, aluminium 2700
The item most easily missed in the database is the "condition" column. Q235 is in the normalised condition and 45 steel is quenched and tempered; if "45 steel" is marked as "normalised", σs is only about 355 MPa and the hardness is a whole class lower. The grade and the heat treatment must always be looked up as a pair.

III. Core Calculation Formulas

σ = F / A (tension-compression stress)
σm = (σmax + σmin) / 2 σa = (σmax − σmin) / 2
n_s = σs / σmax (static strength)
n_f = 1 / (σa/σ-1 + σm/σs) (Soderberg fatigue)
ParameterMeaning
σmax / σminMaximum / minimum values in the working stress cycle
σmMean stress, the steady component
σaStress amplitude, the alternating component and the culprit in fatigue
σ-1Fully reversed (σm=0) fatigue limit — note whether it is bending or tension-compression
n_s / n_fStatic strength safety factor / fatigue safety factor

IV. Quick Reference: Properties and Safety Factors of Common Materials

4.1 Quick Reference of Mechanical Properties of Common Materials (quenched and tempered)

Gradeσb (MPa)σs (MPa)σ-1 bending (MPa)HBRelative cost
Q235B (normalised)400235170≤1561.0
35 steel530315220156~2071.2
45 steel650360275217~2551.4
40Cr980785400241~2862.6
42CrMo1080930450285~3203.4
20CrMnTi (carburised and hardened)108085043058~62HRC3.8

4.2 Recommended Safety Factors

Duty conditionn_s (static strength)Explanation
Accurate load and stress calculation, reliable material1.2~1.5General mechanical parts
Estimated load, castings or corrosive service1.5~2.5Cranes, mining equipment
Important applications, serious consequences of failure2.5~4.0Lifting mechanisms, pressure vessels
Fatigue verification (Soderberg)≥1.5Add size/surface factors for alternating load

4.3 Fatigue Limit Estimation Coefficients

Loading modeRelation of σ-1 to σbExample with 45 steel (σb=650)
Bendingσ-1 ≈ (0.40~0.50) σbabout 275 MPa
Tension-compressionσ-1 ≈ 0.7 × bending valueabout 190 MPa
Torsionτ-1 ≈ 0.55~0.60 × bending valueabout 155 MPa
When the fatigue limit cannot be found, the table above is enough for an estimate, but note that locations with stress concentration (keyways, threads, fillets) also require multiplying by the stress concentration factor Kσ (1.5~3.0) and the surface finish factor, and the actual fatigue strength is roughly halved again.

V. Common Errors and How to Avoid Them

Common errorConsequenceCorrect practice
Looking up only σb and using it for static strength verificationDuctile materials are checked against tensile strength, so the safety factor is overstated by a factor of twoAlways use σs for ductile materials; only brittle materials such as cast iron use σb
Using the bending fatigue limit for tension-compressionFatigue strength overestimated by about 43%, and alternating tension-compression parts fail in batchesTake 0.7 of the bending value for tension-compression and 0.55~0.6 for torsion
Expecting a material change to improve stiffnessSwapping 45 steel for 40Cr leaves the deflection almost unchanged — money wastedE of all steels is about 2.06×10⁵ MPa; stiffness can only be improved by changing the section or the structure
Checking only σmax and not σa in fatigue verificationParts with a high mean stress but small amplitude are wrongly judged safe, and the reverse is missedSeparate σm and σa first, then substitute into Soderberg or Goodman
Looking up the table without the heat treatment conditionσs of the same grade differs by a factor of 2~3 and the verification result is completely distortedLook up grade and condition as a pair (e.g. "45 steel, quenched and tempered") and state it in the drawing technical requirements

One-sentence summary of the material property quick reference: first look at the failure mode to decide which figures to look up, then separate σm and σa, and finally trial-calculate with the cheap material and only upgrade when it fails. Remember three figures — static strength depends on σs, fatigue on σ-1 and stiffness on E, and E cannot be changed by changing the grade.

Related 3D models: Ready to build it? Download free 3D models & CAD drawings at MOULDL »
MOULDL · Mechanical Engineering Knowledge Base · free self-study reference for machine designers, 3D CAD models at MOULDL