Chemical composition per GB/T 3190 standard range (reliability: high); mechanical properties are typical values / ranges (reliability: medium) — acceptance is governed by the purchase standard and the mill test certificate.
| Zn | 5.1~6.1 |
| Mg | 2.1~2.9 |
| Cu | 1.2~2.0 |
| Cr | 0.18~0.28 |
| Condition | Tensile MPa | Yield MPa | Elong. % | Hardness |
|---|---|---|---|---|
| T6 temper | approx. 530~570 | approx. 460~500 | ≥7 | approx. 150HB |
Solution 465~475°C + artificial aging 120°C (T6). T73 two-stage aging trades strength for stress-corrosion resistance.
High-strength structures: jigs, dies, aviation parts, high-end pneumatic cylinders, FRC/robot structures.
AA2024 (GB 2A12) duralumin alloy AA6061-T6 aluminium alloy