Chemical composition per GB/T 3190 standard range (reliability: high); mechanical properties are typical values / ranges (reliability: medium) — acceptance is governed by the purchase standard and the mill test certificate.
| Mg | 0.45~0.9 |
| Si | 0.2~0.6 |
| Al | balance |
| Condition | Tensile MPa | Yield MPa | Elong. % | Hardness |
|---|---|---|---|---|
| T5 temper | ≥160 | ≥110 | ≥8 | approx. 60HB |
After extrusion, air-cool quench + artificial aging (T5). Simpler process and less distortion than T6.
Window/door profiles, equipment-cover frames, conveyor aluminium profiles (the Euro-standard 4040 types), and heatsink profiles.