Chemical composition per GB/T 3077 standard range (reliability: high); mechanical properties are typical values / ranges (reliability: medium) — acceptance is governed by the purchase standard and the mill test certificate.
| C | 0.17~0.24 |
| Si | 0.17~0.37 |
| Mn | 0.50~0.80 |
| Cr | 0.70~1.00 |
| Condition | Tensile MPa | Yield MPa | Elong. % | Hardness |
|---|---|---|---|---|
| Carburized + quenched | surface 56~62HRC | — | — | core approx. 25~40HRC |
Carburize at 930°C → oil quench at 820~840°C → temper at 180~200°C.
Small-section carburized parts: small gears, cams, worms, piston pins. Better hardenability and higher core strength than 20 steel.
20CrMnTi carburizing gear steel (GB) AISI 1020 carbon steel (GB 20)