E41-497 · Screw Selection · CNC Lathe Ball-Screw Steel-Band Damage · ★★★
After 1 year of use, small holes (Φ2 mm) appeared in the protection steel band of the X-axis ball screw on the CNC lathe; coolant seeped through the holes into the screw raceway, and the screw surface rusted within a month.
The screw protection steel band (stainless steel SUS304, 0.2 mm thick, 40 mm wide) wears thin at the support edge (about 0.25 mm → 0.1 mm) due to sliding friction against the guide rail during fast Z-axis reciprocation. Chips (iron chips, hardness about HV500) scratch the band surface, forming tiny through-points (≈0.1 mm dia.) that gradually enlarge to Φ2 mm. Coolant (water-based emulsion, pH ≈ 9) seeps through the holes into the screw raceway; the alkaline components and moisture in the emulsion cause rusting (Fe₂O₃·nH₂O) on the screw surface (GCr15). The rust product is expansive, increasing in volume sixfold, blocking the nut ball recirculation passage and causing ball jamming. From the onset of rusting to nut seizure takes about 3 months.
① Upgrade steel-band material: SUS304 → SUS301 (hardness +50%, better wear resistance)\n② Band thickness: 0.2 → 0.3 mm (puncture resistance ×2.25)\n③ Add polyurethane liner at the band support edge (reduce friction wear)\n④ Inspect the protection band monthly (visual + light-transmission check; replace immediately upon detecting a hole)\n⑤ Apply water-resistant grease inside the screw (complex aluminum-base grease, good water resistance)
FT_11 Ball Screw Selection