Spalling of the Work-Hardened Layer on the Ball Screw Raceway Causes Loss of Accuracy (Grinding Burn)

E41-508 · Ball Screw Selection · Ball Screw Grinding Burn and Spalling · ★★★★

Problem Symptom

After two years of running, spalling (depth about 0.003mm) appeared on the raceway surface of a C1-grade precision ball screw, and the accuracy degraded from ±0.002mm/300mm to ±0.008mm/300mm.

Root Cause

Grinding burn was produced when the raceway of the precision ball screw was ground. In finish grinding the grinding wheel (corundum, grit 80#) used too deep a cut (0.03mm) with insufficient coolant, so the instantaneous surface temperature of the raceway rose to about 500℃. The GCr15 steel underwent secondary hardening (white layer, hardness HV1000+) and tempering (dark layer, hardness HV500). The residual stress in the grinding-burnt layer (about 500MPa tensile) generates micro-cracks at the white layer / dark layer interface. Under cyclic contact stress (about 2000MPa) the micro-cracks propagate and the white layer spalls off the substrate (thickness about 0.003mm). After spalling the raceway surface roughness degraded from Ra0.2μm to Ra1.5μm and the contact fatigue life dropped by about 90%, so the accuracy was lost after two years.

Correct Solution

1) Control the grinding process for the ball screw: finish-grinding allowance ≤0.01mm, adequate coolant (pressure ≥0.5MPa);
2) Inspect for grinding burn after grinding by magnetic particle testing or etching (a ball screw with burn must never be used);
3) Inspect the raceway surface hardness (HRC58~62) and residual stress (X-ray diffraction method);
4) Lap and polish the ball screw raceway surface (remove the burnt layer 0.01mm and polish to Ra≤0.1μm);
5) Select branded ball screws (HIWIN / THK, stable grinding process).

Checklist

References

FT_11_Ball Screw Selection