E41-112 · Other Selection · Outdoor Steel Structure in a Northern Winter · ★★★★
At a factory in Northeast China, an outdoor unit suffered brittle fracture of a weld in a -30℃ winter; the crack ran along the weld into the base metal and the equipment collapsed. The fracture surface showed a typical cleavage fracture (no plastic deformation).
The structure used Q235B carbon structural steel, and the design did not consider low-temperature impact toughness requirements. Q235B has an impact energy AKV ≥ 27J at 20℃, but only about 5J at -30℃ (ductile-brittle transition temperature about -10℃). Per GB/T 700, the lower service temperature limit of Q235B is 0℃ (when impact properties are required), and Q235D should be used below 0℃. The -30℃ of a northern winter far exceeds the applicable lower limit of Q235B. The heat-affected zone (HAZ) of the weld has even lower impact toughness than the base metal (about 3J) and becomes the crack initiation site. The initial microcracks propagate rapidly at low temperature, triggering brittle fracture.
① Material selection for northern winter equipment: at a minimum temperature of -30℃, Q235D is required (AKV ≥ 27J @ -20℃)
② Or Q345D/Q355D low-alloy steel (AKV ≥ 34J @ -20℃)
③ Welding procedure: preheat to 100℃ before welding (plate thickness ≥ 25mm) and keep warm for slow cooling after welding
④ Perform a -30℃ low-temperature impact test on the weld (AKV ≥ 27J)
⑤ Design the structure to avoid stress concentration (keep welds away from corners, use fillet transitions)
FT_Machine Design Handbook