Knowledge Base › Selection Error Cases › Insufficient aging treatment of a cast-iron surface plate leading to post-machining deformation (precision layout plate)

Insufficient aging treatment of a cast-iron surface plate leading to post-machining deformation (precision layout plate)

E41-310 · Other Selection · Precision Layout Plate Aging · ★★★★

Problem Description

A precision cast-iron layout plate (2000×1000×200mm) showed 0.08mm of bending deformation 3 months after finish machining, with flatness deteriorating from 0.01mm/m to 0.05mm/m.

Root Cause

The cast-iron plate is made of HT250 and after casting received only rough machining (milling allowance 5mm)→natural aging (only 2 weeks)→finish machining. The casting residual stress is about 80~120MPa, and 2 weeks of natural aging released only about 10% of it. After finish machining removed the surface layer, the internal residual stress redistributed, causing the plate to deform. The deformation amount ΔL=σ×L/E=80×2000/206000≈0.78mm differs from the actual 0.08mm (the actual plate has stiffening ribs and other bending-resistant structures). The theoretical deformation is about 0.1~0.15mm, which agrees with the actual 0.08mm (accounting for the effect of the stiffening ribs). After deformation the plate's guideway mounting face was no longer flat, affecting equipment accuracy.

Corrective Solution

① Aging treatment for large castings: rough machining→natural aging ≥6 months→semi-finish machining→artificial aging→finish machining\n② Or vibratory stress relief: high efficiency (2~4h), reducing residual stress by 70%\n③ Artificial aging parameters: heat to 550℃ (hold 2h per 25mm wall thickness)→cool in furnace to 200℃→air cool\n④ Allow for stress release during finish machining (rough mill first→store for 2 weeks→finish mill)\n⑤ Or switch to a granite plate (natural stone, zero internal stress, good thermal stability)

Checklist

Reference

FT_Machine Design Handbook

Related model download:Understood the principle and ready to try?Go to MOULDL to download related 3D models and CAD drawings for free »