E41-666 · Chain Drive Selection · Chain Joint Fracture · ★★★★
The transition link (spring-lock-plate type) of a conveyor chain fractured in service, and the chain broke at the joint. Inspection found fatigue fracture of the lock plate and the pin had come out.
The lock plate of the transition link (spring-lock-plate joint) is 1.5 mm thick, made of 65Mn spring steel, HRC42–47. Each time the chain passes over a sprocket the lock plate is bent (compressed on the sprocket teeth and springing back afterwards), giving a bending stress amplitude per revolution of Δσ ≈ 350 MPa (estimated from the bending formula σ_b = 6M/bt², with M = force × moment arm). The bending fatigue limit of 65Mn is about 500 MPa (10⁷ cycles); Δσ = 350 < 500, so it looks safe on the surface. But the lock plate was over-spread during installation (installed at 25° instead of 15°, exceeding the permitted 20°), causing 0.05 mm of plastic deformation at its root and thus pre-damage. With bending fatigue plus pre-damage in service, the lock plate fractured at the root after about 5×10⁵ cycles (about 350 h). Once the lock plate fractured, the pin came out of the link-plate hole and the chain broke.
① Do not over-spread the lock plate when installing the transition link (spread angle ≤ 20°)\n② Use the transition-link lock plate only once (it must be replaced after removal)\n③ Avoid transition links in high-speed or heavily loaded duty\n④ For heavily loaded chains use a cotter-pin joint (more reliable)\n⑤ Inspect the chain joint every shift (lock plate in place, no looseness or cracks)
FT_Belt & Chain Drive Design