E42-263 · Fatigue Fracture · Bed Cast Steel · ★★★
Bed cast steel (ZG270-500) weld repair zone cracks after stress-relief annealing; in service 6 months cracks propagate along weld and fracture; 3 shutdowns per month
[Reheat Crack] After weld repair, mistakenly used 650℃ long-time annealing; Cr-Mo steel in 580~650℃ sensitive range precipitates carbides, weakens grain boundaries, producing reheat cracks.
[Fatigue Propagation] Working alternating stress σ=150MPa superimposed on weld reinforcement stress concentration Kt=2.0; crack growth rate da/dN=3e-7mm/cycle; grows to critical size in service.
[Design Omission] No preheat before weld repair; annealing curve not customized per material; safety factor 1.2 (should be ≥1.8); no weld repair procedure qualification.
1) Preheat 150℃ before weld repair, interpass temperature ≥120℃;
2) Replace long-time annealing with 300℃×2h dehydrogenation treatment;
3) Select low reheat-crack-sensitive welding consumable J507RH;
4) Grind weld bead smooth transition, reinforcement ≤1mm;
5) Customize annealing curve for ZG270-500 and keep ≤580℃;
6) UT+MT inspection after weld repair;
7) Sampling inspect weld repair zone hardness each batch;
8) Re-inspect by flaw detection every 6 months in service.
NB/T 47015-2011