E42-372 · Fatigue Fracture · 08B Roller Chain Link Plate · ★★
08B chain link plate pin hole cracks; chain breaks and stops; 3 repairs per month
[Hole Edge] Pin hole stress concentration Kt=2.3; hole edge σ=310MPa.
[Fatigue] Life 1.5×10⁶ cycles (design ≥1×10⁷).
[Design Omission] Hole not strengthened; plate thickness too small; safety factor 1.3.
1) Ream pin hole and extrusion-strengthen;
2) Increase link plate thickness by 0.5mm;
3) Add boss around hole;
4) Fatigue life check;
5) Magnetic particle test each batch;
6) Improve lubrication;
7) Limit load;
8) Periodic NDE.
GB/T 1243-2006