E42-374 · Fatigue Fracture · Metro Bogie Frame · ★★★
Metro bogie frame side beam weld seam crack 40mm long; speed restricted; 2 trains inspected per month
[Weld Seam] Side beam fillet weld Kt=2.0; alternating σ=180MPa.
[Fatigue] Life 6×10⁶ cycles (design ≥1×10⁷).
[Design Omission] Weld not ground; no stress peak avoidance; safety factor 1.3.
1) Grind weld smooth to R3;
2) Peen weld toe;
3) Upgrade base metal to Q345C;
4) Fatigue check;
5) Magnetic-particle inspect each train;
6) Vibration-damping design;
7) Limit speed;
8) Periodic NDE.
TB/T 1335-1996