E42-379 · Fatigue Fracture · ZLY Hardened Gear Shaft · ★★★
ZLY gear shaft (Φ50) fractures; entire gearbox scrapped; 1 unit repaired per month
[Stress] Shoulder fillet r=1mm, Kt=2.6; σ=380MPa exceeds fatigue.
[Shaft Fracture] Life 2×10⁶ cycles (design ≥1×10⁷).
[Design Omission] Fillet too small; not nitrided; safety factor 1.2.
1) Shoulder fillet R≥3mm;
2) Surface nitriding 0.3mm;
3) Raise shaft diameter to 55mm;
4) Fatigue check;
5) Magnetic-particle inspect each shaft;
6) Dynamic balance;
7) Torque limit;
8) Periodic replacement.
JB/T 8853-2001