Knowledge Base › Structural Design Error Case Study › Molding Sand Gas Evolution on Cast Iron Causing Blowholes and Leakage

Molding Sand Gas Evolution on Cast Iron Causing Blowholes and Leakage

E42-339 · Casting Defects · Cast Iron HT250 · ★★

Problem Description

The casting (HT250) has blowholes Φ5 after machining, leaks hydrostatically; 5 parts scrapped per month

Root Cause

[Blowholes] High sand moisture and high gas evolution; gas cannot escape before solidification.
[Leakage] Blowholes interconnect into channels.
[Design Omission] Sand not controlled, no vents; safety factor only 1.3.

Corrective Solution

1) Control sand moisture to ≤4%;
2) Add vent pins;
3) Raise pouring temperature to 1380℃;
4) Keep sand permeability ≥80;
5) X-ray inspect each batch;
6) Pressure test;
7) Limit pouring speed;
8) Section the first piece.

Checklist

Reference

GB/T 9439-2010