E42-167 · Heat Treatment Distortion and Cracking · 45 Steel Camshaft · ★★
Cam surface hardness HRC48 (should be 55); soft spots show early wear.
[Uneven Temperature] Coil-to-shaft gap off; local temperature too low, not fully hardened. [Soft Spot] The zone is troostitic, hardness drops 7HRC. [Design Omission] No profiled gap, no temperature control; early wear.
1. Design the coil profiled to the cam.
2. Control coil-to-part gap to ±0.5mm.
3. Add rotation on the hardening machine for uniformity.
4. Closed-loop temperature control by infrared pyrometer.
5. Keep coolant flow and pressure constant.
6. Add tempering to homogenize soft-spot zones.
7. Measure hardness point-by-point and plot distribution.
8. Verify the hardened case metallographically on the first piece.
GB/T 16924-2008