E42-417 · Stress Concentration · 1.5MW Wind Main Shaft Bearing Journal · ★★★
1.5MW wind main shaft (Φ300) bearing journal fillet r=1mm fatigue crack; bearing burned; handled at annual inspection
[Small Fillet] Journal r=1mm (should be ≥5mm); Kt=2.8. [Fatigue] Alternating bending-torsion σ=190MPa; life 50k h (design 120k). [Design Omission] Fillet not ground; not strengthened; safety factor 1.2 (should be ≥2.0).
1) Increase journal r to ≥5mm;
2) Roll fillet;
3) Quench-and-temper shaft;
4) Magnetic-particle each shaft;
5) Limit wind speed;
6) Add vibration monitoring;
7) Bearing condition monitor;
8) Replace at end of life.
GB/T 25390-2010