E42-245 · Thermal Deformation and Thermal Stress · Large Cast Iron Platform · ★★★
After rough machining, the platform warped 0.4mm, requiring multiple stress-relief operations.
[Uneven Cooling] The casting has large wall thickness differences and inconsistent cooling sequence, leaving residual stress σ=120MPa. [Warping] After rough machining removed the surface layer, stress release warped the platform 0.4mm. [Design Omission] No annealing was set and the structure has large wall thickness differences.
1. Stress-relief anneal the casting before rough machining.
2. Design uniform wall thickness in the structure.
3. Add a second annealing between rough and finish machining.
4. Add stiffening ribs to the platform.
5. Aging treatment, natural + artificial.
6. Measure warping for each batch.
7. Full flatness inspection.
8. Prevent deformation during lifting.
JB/T 7974-1999