E42-424 · Thermal Deformation and Thermal Stress · Φ700 Hot Rolling Work Roll · ★★★
Φ700 hot rolling roll cooling water biased to one side, temperature difference 40℃, roll surface thermal crack network 3mm deep with spalling; 2 rolls replaced per month
[Uneven] Single-side cooling, roll surface temperature difference 40℃, thermal stress σ=160MPa. [Thermal Cracking] Alternating thermal shock fatigue spalling. [Design Omission] No uniform cooling and no temperature field; safety factor 1.2 (should be ≥1.8).
1) Circumferential uniform-cooling nozzles on the roll body;
2) Temperature control ≤±5℃;
3) Roll surface hardened layer ≥15mm;
4) Measure temperature for each roll;
5) Limit rolling temperature;
6) Regrind the roll surface;
7) On-line monitoring;
8) Replace rolls at end of life.
GB/T 25825-2010