E42-302 · Impact and Overload Fracture · YT28 rock drill piston · ★★
YT28 rock drill piston (Φ60×320): striking-end spalling 8mm deep; 12 pistons replaced per month
[Impact fatigue] Each strike energy E=60J at 30Hz, end-face contact stress σ=900MPa exceeded material strength.
[Spalling] Hardness HRC58 too hard, insufficient toughness, stress-wave reflection caused corner spalling.
[Design Omission] No end toughness matching, no hardness-gradient control; safety factor only 1.1.
1) Lower end hardness to HRC50-54;
2) Decarburize and toughen the 2mm end section;
3) Polish strike face to Ra0.4;
4) Quench-and-temper full piston to HRC40;
5) UT test each batch;
6) Match impact energy to drill steel;
7) Provide buffer and vibration damping;
8) Mandatory replacement at end of life.
GB/T 3077-2015