E42-329 · Residual Stress Deformation · Powder-coated frame · ★★
Frame warped 2mm after powder coating, assembly gap; 2 pieces scrapped monthly
[Coating stress] Coating shrinkage stress σ=30MPa, thin wall warped.
[Warp] Local deformation.
[Design Omission] No preheat, no thickness control; safety factor only 1.3.
1) Preheat to 150℃ before spraying;
2) Coating thickness even ≤80μm;
3) Add longitudinal stiffeners;
4) Slow cooling after spraying;
5) Flatness check each batch;
6) Limit wall-thickness variation;
7) Symmetric spraying;
8) Mechanical straightening.
GB/T 1771-2007