E43-723 · Thread tolerance and fit error · A galvanized M12 bolt with a 15μm coating but no pitch-diameter allowance, so after plating the pitch diameter exceeded the upper limit and it would not enter the nut · ★★★
An M12 bolt had a hot-dip galvanized coating of 15μm per side, but no plating allowance was left on the pitch diameter during machining; after plating the pitch diameter exceeded the 6g upper limit by 0.03mm, interfered with the nut, and would not screw in.
[Mechanism] Thread plating adds thickness to the flanks and increases the pitch diameter; if no plating allowance is left during machining, the post-plate pitch diameter is out of tolerance, interferes with the nut, and will not assemble.
[Calculation] A 15μm per-side coating raises the pitch diameter by about 0.06mm (coating ×4/√3); after plating it exceeds the 6g upper limit by 0.03mm and interferes.
[Design Omission] The pre-plate pitch diameter was not reduced for the coating; this design defect → prevents assembly after plating.
1) Pre-reduce the thread pitch diameter for the coating thickness before plating (about 4t/tan);
2) Recheck with ring gauges after plating;
3) Keep the coating thickness uniform;
4) On the first article, check mating after plating;
5) Optionally tap the nut after plating;
6) Design the coating and tolerances to match;
7) State the coating and pitch diameter on the drawing;
8) Verify mating.
GB/T 197-2018 General-purpose metric screw threads — Tolerances