E43-728 · Thread Tolerance and Fit Error · A 42CrMo threaded part grew 0.04mm past the 6g upper limit after quenching, would not screw into the nut, and had to be re-turned after tempering · ★★★
After quenching a 42CrMo external thread, the pitch diameter grew 0.04mm past the 6g upper limit, interfering with the 6H nut so it would not screw in; the cause was that no heat-treatment distortion allowance was left before quenching.
[Mechanism] Quenching changes volume and distorts the thread, enlarging the pitch diameter; if no distortion allowance was left before quenching, the thread comes out over tolerance and will not screw in.
[Calculation] The 0.04mm pitch-diameter growth on quenching exceeds the 6g upper limit by 0.01mm, interferes with the nut, and prevents entry.
[Design Omission] The pre-quench pitch diameter was not reduced by the expected distortion - a design defect leading to no entry after quenching.
1) Reduce the pre-quench thread pitch diameter by the expected distortion;
2) Stabilize the quench process to control distortion;
3) Grind or repair the thread after quenching when needed;
4) On first articles, measure the post-quench pitch diameter;
5) Recheck with a thread ring gauge;
6) Temper to stabilize dimensions;
7) Note distortion compensation in the process sheet;
8) Verify mating.
GB/T 197-2018 General-purpose metric screw threads — Tolerances