E43-758 · Thread Tolerance and Fit Error · Local plating buildup of 30μm on a galvanized bolt pushes the local pitch diameter out of tolerance, and the thread sticks where the buildup is · ★★★
On a galvanized bolt, plating built up locally at the thread root to 30μm (elsewhere 10μm). The local pitch diameter went out of tolerance; when the thread reached the built-up section it stuck and would not turn, and forcing it damaged the threads.
[Mechanism] Uneven plating makes the local thread thickness out of tolerance; on reaching the built-up section, the pitch diameter interferes and the thread sticks.
[Calculation] A local 30μm plating adds 0.12mm to the local pitch diameter, pushing it past the upper limit into interference and causing sticking.
[Design Omission] The electroplating thickness was uncontrolled and uneven — a process defect leading to local sticking.
1) Control plating uniformity (fixture design / current distribution);
2) Recheck the full length with a GO ring gauge after plating;
3) Keep the plating thickness within the reserved allowance;
4) On first articles, test full-length mating;
5) If needed, rework the threads after plating;
6) Pre-reduce the pre-plating pitch diameter;
7) State the plating-thickness tolerance on the drawing;
8) Verify mating.
GB/T 197-2018 General-purpose metric screw threads — Tolerances