E43-384 · Welded/Cast Forming Dimensional Error · A drive drum ø500mm, designed roundness 0.2, measured post-weld lobing 1.2 · ★★
Weld buckling of the drum shell pushes roundness 1.2mm out of tolerance, causing belt mis-tracking.
[Mechanism] Thin-shell circumferential weld shrinkage buckles the shell into a polygon, pushing roundness out of tolerance.
[Calculation] Polygonization Δ≈0.1·t·(D/t)^1.5/...≈ measured 1.2 (insufficient stiffness), 6× the tolerance of 0.2.
[Design Omission] No internal support or low-stress welding — a design defect leading to roundness error.
1) Use an internal support fixture during welding to hold roundness;
2) Use low current and low heat input;
3) Weld symmetrically in segmented skip passes;
4) Round-up after welding;
5) Add ring stiffeners;
6) Control the sequence;
7) Measure roundness with a caliper gauge;
8) Measure first-article roundness ≤0.2mm.
GB/T 10595-2017 Belt conveyors