E44-984 · Vessel Strength and Wall-Thickness Deficiency · Pressure vessel · ★★★
Hydrogen crack, blister, fracture
[Mechanism] In a wet H2S service, atomic hydrogen diffuses into the steel, combines at inclusions into molecular hydrogen, and forms stepped cracks and blisters.
[Calculation] H2S=50ppm, H in steel=5ppm, CLR=18% exceeds the 15% HIC acceptance, stepped crack 12mm long.
[Design Omission] No H-resistant steel chosen, no H2S control, and no HWTT.
1) Choose HIC-resistant steel (Q345R-HIC, Ca-treated clean steel), since plain carbon steel at CLR 18% fails and a better steel lowers it — thus resisting H;
2) Hold feed H2S≤20ppm (desulfurize), since corrosion rises with concentration and fluid control suppresses cracking — thus suppressing H;
3) Post-weld dehydrogenation (250℃×2h to drive off H), since accumulated H blisters and driving it off disperses it — thus preventing blisters;
4) Control hardness (HAZ≤200HB), since hardness cracks and controlled hardness eases it — thus lowering hardness;
5) Run an HIC test (accept CLR≤15%), since without testing resistance is unknown and the H test verifies it — thus grading resistance by data;
6) Ultrasonic thickness-test for blisters (no blister at any point), since blisters first show as protrusions and can be rejected early — thus finding blisters;
7) Hold operating pH≥9 (suppress H release), since acidity promotes H and alkalinity eases it — thus running to prevent H;
8) Write H-resistance and quality control into the spec, since the hydrogen-crack root cause was the missed H-resistant steel and high H2S — thus locking it in by specification.
GB/T 150.1-2011 Pressure vessels