E44-996 · Vessel Strength and Wall-Thickness Deficiency · Lining · ★★★
Lining delamination, blister, leak
[Mechanism] The bond between lining and substrate failed; under pressure/temperature the lining delaminated and blistered, and the medium seeped in to corrode the substrate.
[Calculation] Bond strength 0.5MPa below operating 1.2MPa, delaminated area 30%, blister height 40mm.
[Design Omission] The lining was not fully bonded, no leak test, and no anchoring.
1) Re-bond the lining (blast Sa2.5 + full adhesive coat), since bond failure delaminates and a sound bond prevents it — thus preventing delamination;
2) Qualify the bonding process (pull-off ≥2MPa acceptance), since a wrong process delaminates and a qualified process is standard — thus bonding firmly;
3) Add anchor points (weld studs every 200mm), since a loose lining delaminates and anchoring holds it — thus anchoring;
4) Perform lining leak testing (spark 5kV over the whole surface), since delamination leaks and the test reveals it — thus finding delamination;
5) Ultrasonic-test blisters (height ≤3mm at every point), since blisters first show as protrusions and can be rejected early — thus finding blisters;
6) Run a bond pull-off test (3 points per zone), since without testing the bond strength is unknown and the test verifies it — thus grading bond by data;
7) Hold heat-up/cool-down rate ≤20℃/h (sudden changes damage the bond), since abrupt change delaminates and a slow rate is steady — thus keeping the bond stable;
8) Write the bonding and bond check into the process card, since the lining-delamination root cause was the missed bond and unchecked lining — thus locking it in by process.
GB/T 150.1-2011 Pressure vessels