E46-070 · Heat Treatment & Stress · 40Cr Forging · ★★★
A 40Cr forging was annealed with the temperature exceeding 850℃ and reaching 1000℃ and a long hold; grain-boundary oxidation and burning occurred, it shattered on hammer impact, and the whole lot was scrapped.
[Mechanism] Heating far above the transformation temperature oxidizes and melts the grain boundaries (burning), and the material loses its toughness completely.
[Calculation] The burning temperature approaches the melting point and an oxide network forms at the grain boundaries, which cannot be remedied.
[Design gap] No temperature upper-limit alarm or dual-thermocouple measurement was provided.
① Set a temperature upper-limit alarm: fit the heating furnace with an audible and visual over-temperature alarm to prevent burning
② Dual-thermocouple measurement: use two thermocouples to cross-check each other and ensure accurate temperature control
③ Control the heating curve: heat according to the process curve and avoid overshoot
④ First-piece check: metallographically inspect the first piece of every furnace charge to confirm it is not burned
⑤ Isolate suspect batches: isolate the whole charge for re-inspection when the temperature is abnormal
⑥ No rework: parts confirmed burned must be scrapped to keep them from flowing on
⑦ Quality verification: confirm by metallography that there is no oxide network at the grain boundaries
⑧ Standardize process: write the temperature upper limit and the alarm into the process card, controlling at the source
GB/T 16923-2008 Normalizing and annealing of steel