E46-261 · Machining Process · CNC Milling Machine · ★★
An aluminum alloy thin plate was milled without coolant; the machining heat arched the middle of the plate up 0.2mm, and after milling and cooling it took a saddle shape, exceeding the flatness tolerance and needing re-milling.
[Mechanism] Cutting heat expands the thin plate locally; uneven contraction on cooling leaves residual distortion.
[Calculation] A temperature rise of 40℃ expands the aluminum plate by about 0.1mm/m, and under constraint the thin plate arches.
[Design gap] Thin-plate machining was done without temperature control or cutting-fluid cooling.
① Add cooling: control the temperature of thin-plate machining with a high-flow cutting fluid
② Small depth of cut: remove the stock in layers with a small depth of cut on thin plates
③ Vacuum clamping: use a vacuum table for even holding to prevent warping
④ Symmetric milling: use symmetric passes to distribute the thermal distortion evenly
⑤ Measure temperature: measure the plate temperature during machining to prevent overheating
⑥ Clamp flat: shim the workpiece solidly when clamping to prevent local looseness
⑦ Flatness verification: confirm flatness with a surface plate or CMM
⑧ Standardize process: write the thin-plate cooling requirement into the process card, controlling at the source
GB/T 1184-1996 Shape and position tolerances - Undefined tolerances