E41-322 · Motor Selection · Field Welded Motor Base · ★★★
The field-welded motor base distorted after welding, and after the motor was installed the shaft axis was offset by 0.12mm (≤0.05mm required). The base had been machined to size before welding, so the distortion forced rework.
The motor base is welded from channel sections (I20a), with the welds concentrated on one side (the fillet welds between the gusset plates and the base plate). The uneven distribution of welding heat causes the base to bend (the welded side contracts on cooling, producing a bending moment). The distortion is δ=α×L×ΔT/2=12×10⁻⁶×800×200/2≈0.96mm (a temperature rise of about 200℃ in the weld zone, base length 800mm). The actual distortion is about 0.12mm because the bending stiffness of the channel limits it. Once the base has distorted the mounting face is no longer flat, so a local gap of about 0.1mm appears between the motor feet and the base. It was roughly aligned using shims, but the shims creep during service and the axis offset gradually grew to 0.12mm.
1) Motor base welding process: weld symmetrically (weld both sides simultaneously to reduce thermal distortion)
2) Welding sequence: weld the central gusset first → then the end gussets (segmented back-step welding method)
3) Stress relief after welding: vibration ageing or natural ageing for ≥48h
4) Re-machine the base mounting face after welding (flatness ≤0.05mm)
5) Or use a bolted base (no welding distortion problem)