E41-075 · Screw Selection · Equipment Maintenance Screw Replacement · ★★
An overstocked screw (Ø40 mm, length 1600 mm) bent due to improper storage (radial runout 0.15 mm). The maintenance shop cold-straightened it with a press and reinstalled it. But after one week of use the screw bent again to 0.20 mm, even worse than before straightening.
Cold-straightening principle: a press applies reverse pressure at the highest point of the bend, plastically deforming the screw to cancel the original bend. But cold straightening introduces new residual stresses inside the screw (compressive in the compressed zone, tensile in the stretched zone), which sit in an unstable equilibrium. Under operating bending stress (~50 MPa) superimposed on the residual stress, when the total exceeds the material elastic limit the screw re-deforms. Residual stress after cold straightening can reach 200~300 MPa (about 30~40% of yield), and releases under minor vibration and thermal cycling. After about 2000 stress cycles (one week of running) the residual stress gradually releases, returning the screw to its original — or even greater — bend.
① Cold straightening of a bent screw is prohibited (it creates unstable residual stress)
② Correct method: hot straightening (heat to 200~300℃ + pressure + hold and slow cool)
③ After hot straightening, perform stress-relief annealing (160℃, hold 4~6 h)
④ Post-straightening check: radial runout ≤0.03 mm, full-length hardness variation ≤HRC2
⑤ If the bend exceeds 0.2 mm/m, scrap and replace with a new screw (straightening cost approaches that of a new part)
⑥ Inventory screw storage: hang vertically or support horizontally (one support point per 500 mm), protect with rust-preventive oil
FT_11 Ball Screw Selection