Knowledge Base › Selection Error Cases › Improper screw material heat treatment causes in-service deformation (custom precision ball sc

Improper screw material heat treatment causes in-service deformation (custom precision ball screw)

E41-074 · Screw Selection · Custom Machine-Tool Screw · ★★★★

Problem Description

A custom non-standard ball screw (Ø50 mm, length 1800 mm) passed incoming inspection, but after one month of installation and use it bent (radial runout increased from 0.02 mm to 0.12 mm). No obvious impact marks were seen on the screw surface.

Root Cause

The screw material is 40CrMo, specified as quench-and-temper (HB280~320) followed by high-frequency induction hardening (HRC58~62), but the heat-treatment execution was flawed: tempering was delayed after quenching (left over 4 h) and the tempering temperature was too low (160℃ → should be 180℃). This left large residual stresses inside the screw (~200 MPa). After about 200 h of operation post-installation, the screw released stress under the combined action of residual and working stresses (bending + thermal), producing bending deformation. Inspection also showed severely non-uniform hardness along the screw length (HRC62 at one end, HRC48 at the other), indicating unstable quenching. The lower-hardness zones have poor wear resistance and showed visible wear after only one month.

Corrective Solution

① Screw material heat treatment: 40CrMo quench-and-temper + medium-frequency induction hardening + low-temperature tempering
② Process requirement: temper within 2 h after quenching, tempering temperature 180℃, hold 4 h
③ Hardness check: full-length hardness variation ≤HRC3, average HRC58~62
④ Straightening process: hot straightening (heat to 200℃ and straighten under pressure); cold straightening prohibited
⑤ Incoming inspection: every screw gets a radial-runout check (≤0.03 mm) + hardness check
⑥ Stress relief: add one artificial aging after tempering (heat to 160℃, hold 8 h, slow cool)
⑦ Manufactured by a professional screw maker; custom parts require a full-dimensional inspection report and heat-treatment report

Checklist

Reference

FT_11 Ball Screw Selection

Related model download:Understood the principle and ready to try?Go to MOULDL to download related 3D models and CAD drawings for free »
MOULDL · Mechanical Engineering Knowledge Base · free self-study reference for machine designers, 3D CAD models at MOULDL