E41-189 · Screw Selection · Precision-Class Screw Use · ★★★★
After 3 months in storage, a C1-class precision screw developed a natural bend of 0.05mm, failing to meet the 0.01mm straightness requirement. Inspection found residual stress inside the screw.
The screw material is GCr15 bearing steel, processed through spheroidizing annealing → quenching → low-temperature tempering → straightening → lapping. The straightening step corrects screw bend at room temperature by local plastic deformation, but it introduces residual stress (about 200~300MPa) inside the screw. After 3 months of natural aging, the residual stress is slowly released; the internal stress redistributes and bending deformation occurs. For a precision screw, deformation from residual-stress release can reach 0.03~0.05mm.
① Precision screws must be stabilized before finish machining\n② Stabilization: quenching → cryogenic treatment (-80℃×2h) → tempering → straightening → artificial aging (150℃×4h)\n③ Or use natural aging: store 3~6 months after rough machining before finish machining\n④ Store vertically suspended (avoid horizontal storage, which worsens bending under self-weight)\n⑤ Check straightness before use; if out of tolerance, re-straighten plus artificial age
FT_11 Ball Screw Selection