E41-338 · Screw Selection · Heavy Lathe Screw Shaft-End Fracture · ★★★★
The heavy lathe X-axis screw fractured at its shaft-end thread relief groove; the R0.3mm (sharp corner) groove showed clear fatigue striations. The fracture was about 50mm from the shaft end.
The screw shaft-end relief groove (R0.3mm sharp corner) has a stress concentration factor Kt≈3.5 (sharp-corner groove). The screw carries an axial tensile force F=12000N (heavy cutting); the nominal stress at the groove σ_nom=F/A=12000/(π×0.015²)=17MPa. Peak stress σ_peak=Kt×σ_nom=3.5×17=59.5MPa. The material is 40Cr (quenched and tempered, σ_b=980MPa, σ_s=785MPa), with fatigue limit σ-1≈350MPa, giving a static safety factor of 13 and a fatigue safety factor of 5.9 — seemingly adequate. But turning produced about 0.02mm-deep tool marks on the groove surface; at the bottom of the marks the stress concentration factor rose further to Kt_total≈5.5, giving an actual peak stress ≈93.5MPa. The alternating load during cutting (cutting→retract cycle) was about 300/day, about 220,000 over 2 years, and a fatigue crack initiated at the tool marks on the groove surface and propagated to fracture.
① Relief-groove fillet radius R≥2mm (drops Kt from 3.5 to 1.5)\n② Surface rolling strengthening of the relief groove (induces compressive residual stress, fatigue strength up 50%)\n③ Or eliminate the relief groove (use a grinding runout relief with fillet R≥5mm)\n④ Switch to a rolled thread at the shaft end (no relief groove, better fatigue resistance)\n⑤ Periodic magnetic-particle inspection (check the screw shaft-end relief groove every 6 months)
FT_11 Ball Screw Selection