Knowledge Base › Selection Error Cases › Improper repair after bearing ring rotation (journal chrome plating) causes recurrence of failure

Improper repair after bearing ring rotation (journal chrome plating) causes recurrence of failure

E41-396 · Bearing Selection · Improper Journal Chrome-Plating Repair · ★★★

Problem Description

A journal (Φ80 mm, worn 0.15 mm) that had experienced bearing ring rotation was repaired by chrome plating; the plating layer was 0.2 mm thick and ground to Φ80k6. After 2 months of operation the chrome layer spalled and ring rotation recurred.

Root Cause

After journal wear, chrome plating was used for repair (plating layer 0.2 mm thick, ground to Φ80k6 after plating). Chrome-plating process: bath temperature 55 ℃, plating solution (chromic acid CrO₃) concentration 250 g/L. The bond strength between the chrome layer and the base material (45 steel) is about 200 MPa; chrome-layer hardness HV900; surface roughness Ra0.2 μm after grinding. During operation at 3000 rpm, the contact stress at the bearing inner-ring/journal fit surface is σ_c≈100 MPa (stress from the interference fit). 100 MPa<200 MPa, so theoretically the chrome layer should not spall. However, before chrome-plating repair the journal base material was not adequately pre-treated (the fatigue layer and oil contamination were not removed), so the actual bond strength between the chrome layer and base material was only about 80 MPa. The fretting stress generated during operation (about 50 MPa) plus the interference stress (100 MPa) gave a total stress of about 150 MPa>80 MPa, causing local spalling of the chrome layer. Spalled chrome fragments (hardness HV900) entered the bearing raceway and aggravated wear.

Corrective Solution

① Journal chrome-plating repair process: turn off the fatigue layer (0.1 mm) → chrome plate (0.3 mm) → grind to size\n② Pre-plating surface treatment: sandblasting + chemical degreasing + acid activation (ensure bond strength)\n③ Chrome-layer bond-strength inspection: bend test or thermal-shock test\n④ Alternatively, use thermal spraying for repair (WC-Co coating, bond strength ≥70 MPa, wear-resistant)\n⑤ Or replace with a new shaft (simple and reliable, avoids repair risk)

Checklist

Reference

FT_23_Bearing Selection Specification

Related model download:Understood the principle and ready to try?Go to MOULDL to download related 3D models and CAD drawings for free »
MOULDL · Mechanical Engineering Knowledge Base · free self-study reference for machine designers, 3D CAD models at MOULDL